Materials Science of Recyling

The Metallurgy of Returning Metal: Impurity Thermodynamics, Microstructure Tolerance, and Alloy Design for Circularity

Metals production is the largest single industrial contributor to global warming. Roughly two billion tonnes of metal are produced annually from more than three billion tonnes of mined minerals, consuming about 10 percent of global energy and generating close to 40 percent of all industrial greenhouse gas emissions, with tailings, slags, dusts and overburden exceeding the metal mass itself by a factor of 15 to 20 [2]. The burden is distributed very unevenly. Steel accounts for about 8 percent of global carbon dioxide emissions, with the blast furnace and basic oxygen converter route emitting 1.8 to 2.2 tonnes of CO2 per tonne of crude steel and still supplying roughly 70 percent of production. Primary aluminium averages about 14.4 tonnes of CO2 per tonne of metal, ranging from below 1 tonne where electrolysis runs on hydropower to about 25 tonnes where it runs on coal-fired electricity. Nickel and cobalt, extracted from ores containing 1 to 2 percent metal, reach 20 tonnes of CO2 per tonne and locally far more [2,3].
 
The physical origin of this asymmetry between primary and secondary synthesis is straightforward and governs everything that follows. Primary extraction is a reduction problem: the metal is chemically bound to oxygen or sulfur, and the free energy of that bond must be paid back. For hematite the thermodynamic minimum is about 6.1 MJ per kilogram of iron, while industrial practice consumes 18 to 25 MJ per kilogram, an efficiency of 22 to 33 percent [2,29]. Aluminium oxide melts above 2000 degrees C and cannot be carbothermically reduced without carbide formation, so it is dissolved in molten cryolite at 950 to 970 degrees C and electrolysed at 13 to 15 kWh per kilogram, with consumable carbon anodes converting the liberated oxygen directly into CO2. Secondary synthesis is a melting problem, not a reduction problem. The metal is already in its reduced state, so only sensible heat and latent heat are required. Aluminium scrap melts at 660 degrees C at roughly 5 percent of the primary energy demand, a saving of up to 95 percent. Steel scrap melted in an electric arc furnace at best practice consumes about 350 kWh per tonne and emits 0.1 to 0.2 tonnes of CO2 per tonne with low-carbon electricity, against 1.8 to 2.2 tonnes for the ore-based route. Per kilogram of steel made from scrap instead of pig iron, about 1.5 kg of CO2, 13.4 MJ of primary energy and 1.4 kg of iron ore are avoided [3]. Because no chemical reductant is needed, scrap melting is also the fastest route to electrifying metallurgy: the blast furnace cannot be electrified, since coke serves simultaneously as reductant, heat source and the load-bearing skeleton that maintains gas permeability in the cohesive zone.
 
The constraint is not thermodynamic but statistical. Steel products remain in service for decades, buildings and bridges for a century; more than 75 percent of all steel ever produced is still in use. Global end-of-life recycling rates for carbon steel are near 60 percent, yet the recycled fraction in new products is only about one third, because demand exceeds scrap availability by roughly a factor of two. Market projections place the scrap share at 45 to 70 percent by 2050, with the wide range reflecting assumptions about product lifetime and stock saturation [3,13]. Aluminium follows a similar trajectory. Even under optimistic assumptions, at least one third of the mass market will remain primary until about 2060, and entropic losses in melting, oxidation, corrosion and dissipation set a hard floor below 100 percent circularity [2,14]. A second constraint is quality. More than half of the carbon steel scrap stream today is old, mixed, post-consumer scrap, and this fraction is projected to exceed 70 percent. In aluminium, most returning scrap is likewise contaminated post-consumer material rather than sorted, in-production runaround scrap. The consequence is that most scrap is currently downcycled into construction grades rather than upcycled into high-performance sheet, and the alloying value embodied in chromium, nickel, molybdenum and niobium is lost to slag or diluted into products that do not need it. Losses of these elements can reach 93 percent when steels are mixed indiscriminately, whereas parts-based sorting can reduce inherent value losses to a few percent [12].
 

Why impurities stay: the thermodynamics and kinetics of scrap refining

Whether a tramp element can be removed from a melt is decided almost entirely by its oxygen affinity relative to the base metal, its vapour pressure, and its solubility in slag. Elements less noble than iron, such as silicon, aluminium, manganese, magnesium and calcium, oxidise readily and partition into slag. Zinc and lead have high vapour pressures and can be evaporated, although manganese co-evaporates and must be replaced. Phosphorus requires oxidising conditions and basic, CaO-rich slag, and must therefore be removed in the converter or electric arc furnace before tapping. Sulfur requires the opposite, reducing conditions and low oxygen potential, and is removed in the ladle furnace. This incompatibility means that a single reactor cannot remove both, and process sequencing is fixed by thermodynamics rather than by convenience [3].
 
The problematic elements are those that are more noble than the base metal and insufficiently volatile. Copper, nickel, cobalt, molybdenum, tin, tungsten, arsenic and antimony cannot be oxidised out of liquid steel without oxidising the iron itself. Copper is the archetype. Its vapour pressure is orders of magnitude below that of zinc at steelmaking temperatures, so vacuum distillation is slow and energy-intensive; effective removal would require repeated remelting under high vacuum, with additional base-metal losses, at a specific energy cost prohibitive for sheet grades [9]. Kinetic simulations of the ladle furnace using the effective equilibrium reaction zone approach, in which the size of the reaction zone sets the mass-transfer rate, show copper content remaining essentially unchanged at 0.35 wt.% over the entire treatment, with only marginal dilution from copper-free ferroalloy additions [3,32]. The same is true of phosphorus under ladle conditions. Industrially, the only viable control is upstream sorting or dilution with direct reduced iron or pig iron, which reintroduces primary emissions and, in the case of pig iron, carbon that must then be oxidised away again.
 
The numbers explain why this matters. Sheet steel specifications typically limit copper to 0.15 wt.% or below and tin to 0.02 wt.%, while long products tolerate up to about 0.4 wt.% copper. Surveys of steel bars produced from scrap in Japan found copper averaging 0.25 to 0.5 wt.%, and the sum of copper, nickel, chromium, molybdenum and tin is now used as a scrap quality index [10,11]. Tinplate carries about 4 kg of tin per tonne of steel; 20 kg of tin in a 100 tonne melt already exceeds the admissible limit. Galvanised sheet carries about 2.8 wt.% zinc. Copper enters vehicles at roughly 20 kg in a combustion car, 40 kg in a hybrid and above 100 kg in a plug-in electric vehicle, and the trend is accelerating with electrification of drivetrains, wiring and electronics [3]. Sorting is itself limited by physics of a different kind: during shredding, copper is cold-welded into the iron, so magnetic and density separation cannot recover it, and coatings, solders and fine wires are dispersed below the liberation size.
 
Aluminium presents the mirror image. Iron is more noble than aluminium, so oxidative refining removes aluminium rather than iron, and iron accumulates monotonically through recycling loops. Removal relies on indirect routes such as manganese or chromium doping followed by gravity sedimentation of primary intermetallic sludge, filtration, fractional crystallisation, or three-layer electrorefining, all of which cost energy and yield. Because most alloying and impurity elements have very low solid solubility in aluminium, contamination expresses itself almost immediately as intermetallic phases rather than as solid solution, which makes cast alloys far more forgiving than wrought alloys. Die-casting grades such as AlSi9Cu3 accept around 1 wt.% Fe, whereas wrought 6xxx alloys are typically held below 0.2 to 0.35 wt.%, and high-ductility A356 below 0.2 wt.% [6,15].
 

What tramp elements do in the solid state

The metallurgical consequences of retained impurities fall into four categories that frequently act simultaneously: alteration of phase equilibria and transformation kinetics, formation of second phases with unfavourable size and morphology, segregation to grain and interphase boundaries, and formation of low-melting films.
 
Copper in steel illustrates the last mechanism. During slab reheating and hot rolling between 1000 and 1200 degrees C, iron oxidises to scale while copper, being nobler, is rejected and enriches beneath the scale layer. Local copper can exceed the austenite solubility limit, about 9 wt.% at 1250 degrees C, and because the copper-rich phase melts near 1080 degrees C it forms a liquid that penetrates austenite grain boundaries under the tensile and bending stresses of rolling. The result is surface hot shortness, intergranular cracking and uncontrolled descaling, which in turn disturbs the thermal balance of the rolling schedule [23,24]. The effect is composition-sensitive in ways that are metallurgically exploitable. Nickel raises copper solubility in austenite and suppresses liquid formation, but is expensive and itself a tramp element in other grades. Tin and antimony lower copper solubility and depress the melting point of the copper-rich phase, aggravating the problem. Silicon promotes occlusion of the copper-rich phase into the internal oxide scale, removing it from the metal surface, and boron, carbon and phosphorus reduce grain boundary penetration. Rapid solidification by strip casting bypasses the mechanism entirely by dispersing copper as fine precipitates instead of allowing subscale enrichment, and the same precipitates can later contribute precipitation hardening [3].
 
Tin, antimony, arsenic and phosphorus act mainly through interface segregation. According to the interfacial decohesion framework of Seah and Hondros, larger segregating atoms weaken ferrite grain boundaries more strongly, placing tin and antimony above phosphorus and arsenic in potency [21]. Auger electron spectroscopy by Grabke and co-workers showed that carbon and boron compete with tin for the same boundary sites and, having higher diffusivity, can pre-empt them [22]. This suggests a deliberate countermeasure: boundary passivation by pre-decoration with light interstitials. It also explains a specific vulnerability of interstitial-free deep-drawing steels, where carbon is held below 0.003 wt.% and nitrogen below 0.004 wt.% and the remainder is scavenged by titanium and niobium. Their boundaries are left undecorated and therefore open to tin and antimony segregation. Beyond embrittlement, such segregation alters primary recrystallisation texture, suppressing the {111} fibre that gives Lankford values above 1.25 and promoting (100)[001] and (110)[001] components that are desirable for electrical steels but damaging for formability [3].
 
In the bulk, most tramp elements shift transformation kinetics. Chromium and molybdenum move the pearlite start to higher temperatures and the bainite start to lower temperatures, widening the transformation-inert region and lowering the critical cooling rate for martensite. Hardenability improves, but continuous hardening becomes harder as martensite start and finish temperatures fall. Strong carbide formers such as molybdenum, tungsten and vanadium can produce coarse carbides and brittle Laves, sigma or chi phases, particularly at higher carbon, degrading toughness and weldability. Manganese is benign in moderation and useful as a deoxidiser and sulfur binder, but the emergence of medium-manganese steels with 3 to 12 wt.% Mn creates a new scrap stream that must be kept separate from carbon steel scrap, exactly as stainless steels are separated today [3].
 
In aluminium alloys the dominant mechanism is morphological. Because iron has almost no solid solubility, it forms intermetallics, and the platelet monoclinic beta-Al4.5FeSi phase, appearing as needles in two-dimensional sections, acts as a stress concentrator and crack initiator. Raising iron from 0.4 to 0.9 wt.% in Al-11Si reduced elongation by 32 percent and tensile strength by 5 percent; from 0.8 to 1.2 wt.% in Al-9Si the losses were 67 and 24 percent [15]. Critically, size matters more than fraction: alloys with different iron contents but identical platelet size showed comparable strength and ductility despite different platelet fractions [18]. Manganese correction, the standard industrial remedy, converts platelets into Chinese-script alpha-Al15(Fe,Mn)3Si2, but reported outcomes are inconsistent. Adding 0.2 wt.% Mn to Al-9Si-0.8Fe raised elongation from 4.7 to 6.9 percent, while 0.7 wt.% Mn brought it back to 5.6 percent; 0.73 wt.% Mn in Al-7Si-1.2Fe gave a 168 percent elongation gain, with higher additions again degrading properties [19,33]. The optimum is not a fixed Mn/Fe ratio but a function of composition, cooling rate and the resulting phase selection.
 
For functional applications the relevant impurity metric is electron scattering rather than fracture. In copper, dilute transition-metal solutes are potent scatterers because of spin-disorder effects: reported resistivity coefficients are 10.6 to 12.0 micro-ohm cm per at.% Fe, 2.9 to 3.4 per at.% Mn, 0.6 to 7.3 per at.% Co and about 1.2 per at.% Ni, against an intrinsic resistivity of 1.72 micro-ohm cm for pure copper. Even 0.1 at.% Fe in solution costs roughly 40 percent of the conductivity [4,31].
 

From tolerance to exploitation: three worked examples

The productive shift in recent work is from removing impurities to designing microstructures that accommodate them, and in some cases use them. Three systems illustrate the required reasoning at different levels.
 
Secondary Al-Si casting alloys. Classical Scheil-Gulliver calculations assume infinite diffusion in the liquid, no diffusion in the solid and local equilibrium at the interface, with no nucleation barrier. For substitutional silicon, iron and manganese the neglect of back diffusion is defensible, but the absence of a nucleation model causes systematic errors: predicted beta platelets are frequently replaced in practice by delta-Al4FeSi2, and Chinese-script phases appear where none are predicted [1,16,17]. A more predictive scheme couples Scheil-derived liquid compositions and temperatures to the parallel-tangent precipitation driving force, to solid-liquid interfacial energies estimated by a generalised nearest-neighbour broken-bond model, and to classical nucleation theory with realistic nucleus shapes [1]. The results are quantitative and design-relevant. The critical combined Fe plus Mn content that keeps intermetallics out of the pre-eutectic stage peaks at about 1.1 wt.%, specifically 0.77 wt.% Fe plus 0.31 wt.% Mn, at the eutectic composition near 12.67 wt.% Si, and falls to 0.57 wt.% total at 7 wt.% Si with 0.2 wt.% Mn. At that maximum the corrected fraction, defined as the fraction of Chinese-script phase relative to all iron intermetallics, is only 0.47. Complete correction and complete suppression of pre-eutectic formation are thermodynamically incompatible, which rationalises the industrial practice of partial manganese correction.
 
Experiment then reverses the intuition depending on contamination level. At 0.8 wt.% Fe and about 3 K per second, the near-eutectic Al-11Si alloy achieved a corrected fraction of 0.82 against 0.41 for Al-7Si, with tensile strength 121 against 100 MPa and elongation 3.0 against 2.2 percent, because the platelet driving force turns positive only about 16 degrees C lower in the near-eutectic alloy, leaving less growth time and a narrower undercooling window before the metastable cubic Chinese-script phase forms. At 2.0 wt.% Fe the ranking inverts: the far-from-eutectic Al-7Si alloy showed 133 percent higher elongation and 58 percent higher strength, because the sharp rise in beta driving force at the aluminium dendrite formation temperature of 613 degrees C raises the nucleation rate and refines the platelet dispersion [1]. Cooling rate acts as a third design variable. At about 50 K per second near the mould wall, trigonal gamma-Al3FeSi forms as fine polyhedra instead of beta platelets in both alloys; classical nucleation theory with an oblate spheroidal beta nucleus of aspect ratio 50 gives a barrier more than 20 times that of the spherical gamma nucleus and a critical radius of 25 nm against 2.9 nm, so mobility limits suppress the platelet. Manganese addition of 0.5 wt.% reduced maximum platelet size by 60.3 percent in the near-eutectic alloy and 81.3 percent in the far-from-eutectic alloy at the slower-cooled centre, eliminating coarse beta entirely in the latter, where the undercooling window between alpha-Al15(Fe,Mn)3Si2 and beta is 18 degrees C rather than 3 degrees C, and where a peritectic dissolution step further blocks beta formation. The practical rules that follow are conditional rather than universal: manganese is redundant at high cooling rates, essential at slow cooling, and required in smaller amounts for heavily contaminated far-from-eutectic compositions.
 
Copper current collectors from electric vehicle batteries. Copper foil recovered from spent NMC811 cells carries iron, nickel, cobalt and manganese from cathode and casing contamination. Rather than refining these away, the strategy is to getter them into nanoprecipitates so that the matrix is thermodynamically self-cleaning, and then to tune the precipitate spacing against the conduction electron mean free path [4]. Atom probe tomography showed Fe-Co-rich particles already present in the as-cast state, confirming low solubility. After annealing at 450 degrees C the particles were 3.4 nm in diameter at 1.35 percent volume fraction with 9.2 nm spacing; after 550 degrees C they were 5.4 nm at 0.15 percent with 40.8 nm spacing. The room-temperature phonon-limited mean free path in copper is 40 to 50 nm, so the coarser dispersion is effectively invisible to conduction electrons while the finer one is not. Measured resistivity was 3.94 and 2.68 micro-ohm cm respectively, against 1.74 for commercial foil, corresponding to roughly 45 and 65 percent IACS. Internal structure matters as a second-order effect: the 450 degrees C particles adopt a 9R stacking with stacking faults, the 550 degrees C particles a twinned 3R structure, and twin interfaces scatter about an order of magnitude less strongly than stacking faults. Mechanically, both conditions outperform commercial foil, with yield strengths of 138 and 109 MPa against 79 MPa, tensile strengths of 233 and 215 MPa and elongations above 84 percent, the precipitation contribution being 47 and 34 MPa after subtracting lattice friction, Hall-Petch and dislocation terms. Coin-cell and impedance tests confirmed acceptable rate performance, with the coarser-grained, cleaner-matrix condition favoured at higher C-rates. The conclusion is not that purity is irrelevant, but that the 99.99 percent specification can be relaxed for this application when the impurities are spatially reorganised rather than removed.
 
Ductile iron from 100 percent scrap. Ductile iron accounts for about 120 million tonnes annually, 28 percent of cast iron consumption, and is metallurgically tolerant enough to be a realistic target for full scrap charging, yet conventional practice degrades irreversibly above about 70 wt.% scrap because both strength and ductility fall together. A data-driven approach, coupling a 330-entry composition-processing-microstructure-property dataset from an instrumented production line with a larger 2400-entry composition-property dataset, convolutional surrogate models and a tree-search optimiser constrained to spread candidates along a Pareto front, produced 17 candidates of which 14 improved on the existing front, with gains up to 15.2 percent in tensile strength and 73.2 percent in elongation and an 8.1 percent cost reduction at 100 percent scrap and full recyclability [5]. The mechanisms are conventional but their combination is not. The best variant, at 3.31 C, 2.77 Si, 0.30 Mn and 0.27 Cu in wt.%, reached 590 MPa with 18.5 percent elongation by combining 34.6 percent pearlite with 196 nm interlamellar spacing, 56.2 percent ferrite for crack blunting, and 13.2 percent graphite at 292.8 nodules per square millimetre and 21.25 micrometre mean diameter, finer and more numerous than the expert-designed reference. Impurity-derived Cu-, Ti-, Mg- and Sn-bearing nanoparticles contributed 114 to 152 MPa of Orowan strengthening, and silicon and copper in solution about 148 MPa, with silicon held below 4.3 wt.% to avoid iron-silicon long-range ordering embrittlement. Deviating from the optimised processing window degraded graphite sphericity by 30 percent and increased nodule size by 20 percent, raising local misorientation near the graphite-matrix interface from 3.3 to 5.1 degrees and triggering premature fracture. The lesson is that in heavily contaminated melts the controlling variables are as much thermal history and nodule statistics as bulk chemistry, and that the composition-processing-property mapping is too high-dimensional for intuition alone.
 

Design rules for a circular alloy system

Several principles generalise across these cases. The first is that chemical composition is a conserved quantity while microstructure is not. Every alloying atom added returns to the scrap pool, whereas grain size, phase fractions, precipitate dispersion and defect density can be reset indefinitely by solidification, deformation and heat treatment. This favours an alloy design philosophy of microstructural complexity from chemical simplicity: several hundred steel grades are already accessible within Fe-C-Mn-Si, and lean maraging concepts such as Fe-18Mn-3Ti achieve ultrahigh strength through segregation-controlled nanoprecipitation without nickel, cobalt or molybdenum [2,27]. For aluminium, crossover alloys that blur the boundaries between the 5xxx and 2xxx or 7xxx families combine formability with age hardening and reduce the number of chemically distinct grades that mix during scrapping [25,26].
 
The second is that alloys must be designed simultaneously as acceptors of scrap and donors of scrap. Casting alloys are natural sinks because their properties tolerate coarse second phases better than forming grades do. Wrought sheet, particularly for outer-skin automotive applications, is the hardest acceptor. Reducing alloy variety, collecting runaround scrap in-production, and establishing separate streams for medium-manganese and stainless grades are structural measures with metallurgical consequences, since they determine the impurity spectrum that any alloy design must accommodate [6,14].
 
The third is that specifications should be re-derived rather than inherited. Many impurity limits were fixed for processing conditions that no longer apply. Faster solidification, higher nucleation rates, thinner cast sections and better thermomechanical control disperse harmful phases more finely and dilute boundary segregation over more interface area. Systematic re-examination of tolerance limits, coupled with the recognition that charge-to-charge variability may be more damaging than a higher mean impurity level, argues for designing against the tails of the composition distribution rather than its mean, and for using processing as the compensator. Adjusting intercritical annealing time to offset copper variation in medium-manganese steel, or tempering temperature to accommodate 1 wt.% Cu in 42CrMo4, are concrete demonstrations [3].
 
The fourth is that process design carries as much leverage as alloy design. Near-net-shape and thin-strip casting reduce the required hot deformation from more than 98 percent thickness reduction to a few percent, cutting energy from about 2100 to 200 MJ per tonne, reheating demand from 1.2 to 1.5 GJ per tonne down to 0.1 to 0.5, and rolling electricity from 80 to 100 kWh per tonne down to 30 to 60, while simultaneously suppressing segregation gradients and the copper hot-shortness mechanism [2,3]. Hydrogen plasma smelting reduction has been shown to remove sulfur, phosphorus and even copper from iron melts, offering a refining route that conventional slag practice cannot provide [28]. Sorting is improving through laser-induced breakdown spectroscopy, machine vision and learned classification, but its effectiveness is capped by product design: batteries, magnets and circuit boards must be removable before shredding, or their elements are irreversibly dispersed into bulk scrap [14,35].
 
The limits of the approach should be stated plainly. Impurity-tolerant design applies to engineering alloys where moderate contamination can be managed by phase selection, dispersion and interface engineering. It does not extend to applications where trace contamination is catastrophic, such as semiconductors or certain high-purity functional materials. Data-driven design requires representative datasets and remains unreliable when extrapolating far outside them, which is why closed-loop experimental validation is not optional. And the underlying thermodynamic and kinetic databases are still thin for the multicomponent, impurity-rich systems that recycling actually produces: interfacial energies of iron intermetallics in aluminium melts, nucleation pathways that may be non-classical, grain boundary segregation isotherms in five- and six-component steels, and the interaction of tramp elements with vacancies and dislocations remain incompletely parameterised. These are the measurable gaps that determine whether recycling can move from downcycling construction steel to upcycling safety-critical sheet, conductors and castings at the scale the material cycle requires.
 

 

References

  1. Mohammed, W., Chen, X., Ponge, D., Raabe, D. Thermodynamics-guided design of sustainable secondary Al-Si alloys for enhanced Fe-impurity tolerance and optimized Mn doping. Acta Materialia 289 (2025) 120932.
  2. Raabe, D. The materials science behind sustainable metals and alloys. Chemical Reviews 123 (2023) 2436-2608.
  3. Raabe, D., Jovicevic-Klug, M., Ponge, D., Gramlich, A., Kwiatkowski da Silva, A., Grundy, A. N., Springer, H., Souza Filho, I., Ma, Y. Circular steel for fast decarbonization: thermodynamics, kinetics, and microstructure behind upcycling scrap into high-performance sheet steel. Annual Review of Materials Research 54 (2024) 247-297.
  4. Nutor, R. K., Ruffino, M., Cohen Miles, A., Joshi, Y., Woods, E. V., Bhat, M. K., Jannat, S. R., Manzoor, U., Souza Filho, I. R., Raabe, D., Gault, B. Enabling circularity of copper through nanoscale impurity control. Acta Materialia 297 (2025) 121373.
  5. Yang, C., Peng, B., Sun, B., Tao, Q., Zeng, Y., Zhang, L., Shu, D., Lu, J., Raabe, D., Han, L., Wei, Y. From scrap to prime: designing high-performance alloys from dirty feedstocks with machine learning. Science Advances 12 (2026) eaeg9183.
  6. Raabe, D., Ponge, D., Uggowitzer, P. J., et al. Making sustainable aluminum by recycling scrap: the science of dirty alloys. Progress in Materials Science 128 (2022) 100947.
  7. Raabe, D., Tasan, C. C., Olivetti, E. A. Strategies for improving the sustainability of structural metals. Nature 575 (2019) 64-74.
  8. Daehn, K. E., Cabrera Serrenho, A., Allwood, J. M. How will copper contamination constrain future global steel recycling? Environmental Science and Technology 51 (2017) 6599-6606.
  9. Daehn, K. E., Cabrera Serrenho, A., Allwood, J. M. Finding the most efficient way to remove residual copper from steel scrap. Metallurgical and Materials Transactions B 50 (2019) 1225-1240.
  10. Daigo, I., Tajima, K., Hayashi, H., et al. Potential influences of impurities on properties of recycled carbon steel. ISIJ International 61 (2021) 498-505.
  11. Panasiuk, D., Daigo, I., Hoshino, T., et al. International comparison of impurities mixing and accumulation in steel scrap. Journal of Industrial Ecology 26 (2022) 1040-1050.
  12. Ohno, H., Matsubae, K., Nakajima, K., et al. Toward the efficient recycling of alloying elements from end of life vehicle steel scrap. Resources, Conservation and Recycling 100 (2015) 11-20.
  13. Pauliuk, S., Milford, R. L., Muller, D. B., Allwood, J. M. The steel scrap age. Environmental Science and Technology 47 (2013) 3448-3454.
  14. Reuter, M. A., van Schaik, A., Gutzmer, J., Bartie, N., Abadias-Llamas, A. Challenges of the circular economy: a material, metallurgical, and product design perspective. Annual Review of Materials Research 49 (2019) 253-274.
  15. Taylor, J. A. Iron-containing intermetallic phases in Al-Si based casting alloys. Procedia Materials Science 1 (2012) 19-33.
  16. Becker, H., Bergh, T., Vullum, P. E., Leineweber, A., Li, Y. Effect of Mn and cooling rates on alpha-, beta- and delta-Al-Fe-Si intermetallic phase formation in a secondary Al-Si alloy. Materialia 5 (2019) 100198.
  17. Gorny, A., Manickaraj, J., Cai, Z., Shankar, S. Evolution of Fe based intermetallic phases in Al-Si hypoeutectic casting alloys: influence of the Si and Fe concentrations, and solidification rate. Journal of Alloys and Compounds 577 (2013) 103-124.
  18. Bjurenstedt, A., Seifeddine, S., Jarfors, A. E. W. The effects of Fe-particles on the tensile properties of Al-Si-Cu alloys. Metals 6 (2016).
  19. Song, D., Zhao, Y., Jia, Y., et al. Study of the evolution mechanisms of Fe-rich phases in Al-Si-Fe alloys with Mn modification using synchrotron X-ray imaging. Journal of Alloys and Compounds 915 (2022) 165378.
  20. Cinkilic, E., Ridgeway, C. D., Yan, X., Luo, A. A. A formation map of iron-containing intermetallic phases in recycled cast aluminum alloys. Metallurgical and Materials Transactions A 50 (2019) 5945-5956.
  21. Seah, M. P. Adsorption-induced interface decohesion. Acta Metallurgica 28 (1980) 955-962.
  22. Grabke, H. J. Surface and grain boundary segregation on and in iron and steels. ISIJ International 29 (1989) 529-538.
  23. Kondo, Y. Behaviour of copper during high temperature oxidation of steel containing copper. ISIJ International 44 (2004) 1576-1580.
  24. Shibata, K., Seo, S. J., Kaga, M., et al. Suppression of surface hot shortness due to Cu in recycled steels. Materials Transactions 43 (2002) 292-300.
  25. Stemper, L., Tunes, M. A., Tosone, R., Uggowitzer, P. J., Pogatscher, S. On the potential of aluminum crossover alloys. Progress in Materials Science 124 (2022) 100873.
  26. Cann, J. L., De Luca, A., Dunand, D. C., et al. Sustainability through alloy design: challenges and opportunities. Progress in Materials Science 117 (2021) 100722.
  27. Kwiatkowski da Silva, A., Souza Filho, I. R., Lu, W., et al. A sustainable ultra-high strength Fe18Mn3Ti maraging steel through controlled solute segregation and alpha-Mn nanoprecipitation. Nature Communications 13 (2022).
  28. Souza Filho, I. R., Ma, Y., Kulse, M., Ponge, D., Gault, B., Springer, H., Raabe, D. Sustainable steel through hydrogen plasma reduction of iron ore: process, kinetics, microstructure, chemistry. Acta Materialia 213 (2021) 116971.
  29. Gutowski, T. G., Sahni, S., Allwood, J. M., Ashby, M. F., Worrell, E. The energy required to produce materials: constraints on energy-intensity improvements, parameters of demand. Philosophical Transactions of the Royal Society A 371 (2013) 20120003.
  30. Wang, P., Ryberg, M., Yang, Y., et al. Efficiency stagnation in global steel production urges joint supply- and demand-side mitigation efforts. Nature Communications 12 (2021) 2066.
  31. Gall, D. Electron mean free path in elemental metals. Journal of Applied Physics 119 (2016).
  32. Van Ende, M. A., Jung, I. H. A kinetic ladle furnace process simulation model: effective equilibrium reaction zone model using FactSage macro processing. Metallurgical and Materials Transactions B 48 (2017) 28-36.
  33. Baldan, R., Malavazi, J., Couto, A. A. Microstructure and mechanical behavior of Al9Si0.8Fe alloy with different Mn contents. Materials Science and Technology 33 (2017) 1192-1199.
  34. Lu, X., Zhang, Z., Hiraki, T., Takeda, O., Zhu, H., Matsubae, K., Nagasaka, T. A solid-state electrolysis process for upcycling aluminium scrap. Nature 606 (2022) 511-515.
  35. Harper, G., Sommerville, R., Kendrick, E., et al. Recycling lithium-ion batteries from electric vehicles. Nature 575 (2019) 75-86.
 
Sustainability of structural metals
Raabe_et_al-2019-Nature.pdf
PDF-Dokument [2.2 MB]
Sustainable secondary Al-Si alloys for enhanced Fe-impurity tolerance and optimized Mn doping
Acta Full paper Al Si recycling 01-s_Opt[...]
PDF-Dokument [2.1 MB]
Druckversion | Sitemap
© D. Raabe